Replace Ferrosilicon with Silicon Carbide: A Cost-Saving Guide for Steel Plants
Silicon carbide (SiC) has moved from a niche alternative to a mainstream partial replacement for ferrosilicon (FeSi) in steelmaking. It delivers both silicon and carbon in one addition - deoxidising the bath, contributing to the carbon specification, and generating exothermic energy that improves furnace efficiency. This guide explains the chemistry, the arithmetic, and the practical trial protocol so that a procurement manager or plant metallurgist can evaluate SiC substitution with confidence - not guesswork.
Key Takeaways
One kilogram of 90% SiC delivers approximately 0.63 kg of silicon and 0.27 kg of carbon to the molten bath - you replace two materials with one addition.
Start with 30–50% partial replacement of FeSi silicon units. Full substitution is feasible for plain carbon and rebar grades but not for ultra-low-carbon or tight-specification alloy steels.
Particle size controls dissolution speed. 1–3 mm is the general-purpose choice for ladle additions; 10–50 mm lumps suit BOF converter practice.
Cost savings depend on your local FeSi vs. SiC price spread. Based on late-2025 to mid-2026 Chinese domestic pricing, SiC has traded at an 8–15% discount per equivalent silicon unit.
Monitor deoxidation efficiency, carbon pick-up consistency, and slag fluidity across at least 10 heats before scaling the substitution ratio.

Need a Custom SiC Cost Model for Your Mill?
Send us your current FeSi consumption, target steel grades, and delivered price - our engineering team will build a plant-specific substitution analysis at no charge.
Email: market@zanewmetal.com · WhatsApp: +86 155 1882 4805
1. The Chemistry: How SiC Works in Molten Steel
To evaluate SiC as a ferrosilicon replacement, start with what happens when it enters the bath. Silicon carbide does not simply dissolve - it undergoes two sequential thermochemical processes that distinguish it from FeSi.
1.1 Dissociation and Deoxidation
At steelmaking temperatures (~1,600°C), SiC dissociates. The silicon reacts preferentially with dissolved oxygen (FeO) in the bath:
Si + 2 FeO → SiO₂ + 2 Fe ΔH = −301 kJ/mol Si (exothermic)
The resulting silica (SiO₂) reports to the slag. Because this reaction is exothermic, each kilogram of SiC added provides a modest thermal contribution - a secondary benefit when scrap ratios are high or hot-metal temperature is marginal.
1.2 Carbon Dissolution
The carbon from SiC dissolves into the steel bath:
C (from SiC) → [C] in molten steel
This is the critical difference from FeSi: ferrosilicon delivers silicon only, while SiC delivers both silicon and carbon. For steel grades with a carbon specification above 0.10%, this dual delivery simplifies the addition practice. For grades below 0.06% C, the carbon contribution from SiC must be accounted for and may limit the substitution ratio.
1.3 Slag Interaction
The silica formed during deoxidation (SiO₂) is acidic. In a BOF or ladle furnace with a basic slag (CaO/SiO₂ ratio typically 2.5–3.5), the additional SiO₂ from SiC may shift the slag basicity slightly downward. This is usually benign at partial replacement ratios (30–50%) but should be monitored through slag sampling during the trial phase. When the slag V-ratio (CaO/SiO₂) drops below 2.0, desulfurisation capacity declines - a condition to watch if your plant produces low-sulfur grades.
2. Stoichiometry: What One Kilogram of SiC Delivers
The value of SiC as a FeSi substitute rests on a straightforward mass balance. SiC has a molecular weight of 40.1 g/mol (Si = 28.1, C = 12.0). In pure SiC, silicon is 70.0% by mass and carbon is 30.0%.
Metallurgical-grade SiC is not pure - the balance includes free carbon, silica, and minor oxides. The table below shows the effective silicon and carbon delivered per kilogram for the two common grades.
| SiC Grade | SiC Purity (wt%) | Available Si (kg/kg) | Available C (kg/kg) | Typical Free C (wt%) | Typical SiO₂ (wt%) |
|---|---|---|---|---|---|
| SiC 88% | ≥ 88 | ≈ 0.62 | ≈ 0.26 | ≤ 5.0 | ≤ 5.0 |
| SiC 90% | ≥ 90 | ≈ 0.63 | ≈ 0.27 | ≤ 3.0 | ≤ 3.5 |
Available Si and C are theoretical maxima based on stoichiometry (Si = 28.1 / 40.1 = 70.0%; C = 12.0 / 40.1 = 30.0%) multiplied by SiC purity. Actual recovery in the bath depends on addition practice, slag condition, and stirring - typically 85–95% for silicon and 80–90% for carbon in well-controlled ladle additions. Source: SiC molecular data from NIST Standard Reference Database; impurity ranges per GB/T 2480-2022.
Practical comparison: To deliver 1.0 kg of silicon to the bath, a plant needs approximately 1.59 kg of 90% SiC (assuming 100% theoretical yield) versus approximately 1.33 kg of FeSi75 (75% Si). The SiC route adds roughly 0.43 kg of carbon at the same time - which may reduce or eliminate the need for a separate recarburiser addition. The net economics depend on whether your process wants that carbon.
3. Grade Selection: SiC 88% vs. SiC 90%
The choice between 88% and 90% SiC is not simply a question of purity - it affects recovery predictability, slag volume, and the consistency of carbon pick-up from heat to heat.
| Criterion | SiC 88% | SiC 90% |
|---|---|---|
| Cost per ton (indicative Q2 2026, FOB China) | Lower by ~5–8% | Baseline |
| Silicon recovery consistency | Good; ±3% variation feasible | Better; ±1.5% typical |
| Free carbon content | ≤ 5.0% | ≤ 3.0% |
| Slag volume impact | Slightly higher (more SiO₂ and oxides from impurities) | Lower |
| Recommended application | Rebar (GB 1499.2), wire rod, structural sections, low-alloy plate | Pipeline steel, cold-heading quality, automotive sheet, quality-critical heats |
| GB/T reference | GB/T 2480-2022, black SiC, metallurgical grade | GB/T 2480-2022, black SiC, metallurgical grade |
Prices are indicative and vary with order volume, contract terms, and freight destination. ZhenAn International provides SGS-certified lot assays with every shipment. Compared with ferrosilicon (GB/T 2272-2020, most commonly FeSi75 grade containing 72–80% Si), SiC offers the dual-function advantage at a lower cost per equivalent silicon unit in most market conditions.
4. Particle Size and Absorption Kinetics
Particle size is not a secondary detail - it governs how fast the SiC dissolves, where in the furnace it reacts, and whether fines are lost to off-gas before they reach the bath. The relationship is straightforward: smaller particles dissolve faster but are more vulnerable to dust loss; larger particles survive longer in the slag layer but dissolve more slowly.
| Size Range | Dissolution Time* | Best Application | Key Risk |
|---|---|---|---|
| 0–1 mm | < 10 seconds | Ladle furnace, argon-stirred, enclosed addition system | Fines lost to off-gas extraction before entering bath |
| 1–3 mm | ~15–30 seconds | Ladle furnace (general purpose); most widely used | Acceptable dust loss if added at correct lance depth |
| 3–10 mm | ~30–90 seconds | BOF converter addition; ladle with weak stirring | Incomplete dissolution if added late in the heat |
| 10–50 mm | > 90 seconds | BOF converter (lump addition with scrap or hot metal) | Slower dissolution; ensure addition early in the blow |
*Approximate dissolution time in a 1,600°C bath with moderate argon stirring. Actual time varies with bath temperature, slag depth, stirring intensity, and SiC purity. Source: Fiven ASA technical literature on SIKA® metallurgical SiC; Miller and Company LLC application notes.
The general-purpose recommendation is 1–3 mm for ladle furnace additions. It provides a workable balance of dissolution speed and recovery. Plants adding SiC to BOF converters should use 10–50 mm lump material and add it with the scrap charge or early in the oxygen blow to ensure full dissolution before tapping.
5. Step-by-Step Replacement Protocol
Switching from FeSi to SiC is not a one-time substitution - it is a calibrated process. The protocol below is based on practices validated across multiple Chinese steel plants and aligned with recommendations from Miller and Company LLC and Fiven ASA.
Step 1: Baseline Data Collection (1 week)
Before making any change, record the following for at least 20 consecutive heats using your current FeSi-only practice:
FeSi addition weight per heat (kg)
Tap silicon and carbon (average and standard deviation)
Silicon recovery rate: (Si in tapped steel − Si in scrap/hot metal) ÷ Si added
Slag basicity (CaO/SiO₂) after addition
Final oxygen content (ppm)
Step 2: Partial Substitution Trial (30%, 10 heats minimum)
Replace 30% of the FeSi silicon units with SiC silicon units. Calculate the SiC addition weight as:
SiC addition (kg) = FeSi silicon replaced (kg) ÷ (SiC purity × 0.70)
Example: A plant adds 200 kg of FeSi75 per heat (150 kg Si). Replacing 30% of silicon units (45 kg Si) with 90% SiC requires: 45 ÷ (0.90 × 0.70) = 71.4 kg of 90% SiC. Reduce FeSi addition to 200 − (45 ÷ 0.75) = 140 kg. The net addition becomes 140 kg FeSi75 + 71.4 kg 90% SiC.
Step 3: Scale to 50% (10 heats minimum)
If the 30% trial shows acceptable silicon recovery (within ±5% of baseline) and carbon pick-up is stable, increase to 50% silicon-unit substitution. Monitor the same parameters plus carbon end-point distribution.
Step 4: Optimise and Standardise
After validating at 50%, decide whether to maintain that ratio or push higher based on the steel grade's carbon tolerance. Document the standard operating procedure (SOP) with target addition weights, addition sequence (when in the heat to add SiC), and acceptable tolerance bands for silicon and carbon.
6. Furnace Performance Monitoring During Transition
During the trial phase, monitor three indicators per heat:
| Indicator | What to Measure | Acceptable Range During Trial | Red Flag |
|---|---|---|---|
| Deoxidation efficiency | Final oxygen content (ppm) vs. baseline | ±10% of baseline average | Oxygen > 20% above baseline for 3+ consecutive heats |
| Carbon stability | Standard deviation of tap carbon across trial heats | Within 120% of baseline σ | Carbon overshoot beyond upper spec limit in any heat |
| Slag fluidity | Visual assessment + CaO/SiO₂ ratio from slag sample | V-ratio > 2.0; no skull formation on slag rake | V-ratio drops below 1.8 or slag appears viscous/sticky |
These thresholds are conservative starting points. Each plant should adjust based on its specific steel grades and furnace practice.
7. Cost Framework: Comparing FeSi and SiC on an Equivalent Basis
The most common error in cost comparison is comparing the price per ton of FeSi vs. SiC directly. That comparison is meaningless because the materials deliver different amounts of silicon per ton. The correct metric is cost per kilogram of silicon delivered to the bath, adjusted for recovery.
| Parameter | FeSi75 (GB/T 2272-2020) | SiC 90% (GB/T 2480-2022) |
|---|---|---|
| Silicon content (wt%) | 72–80% (use 75% nominal) | 63% available Si (90% × 0.70) |
| Typical Si recovery in ladle | 90–95% | 85–92% |
| Effective Si delivered (kg per 100 kg material) | ~67.5–71.3 kg | ~53.6–58.0 kg |
| Additional benefit | None | ~24–27 kg carbon per 100 kg (may reduce/eliminate recarburiser) |
| Exothermic contribution | Moderate | Higher (Si + C both oxidise exothermically) |
Recovery rates are indicative and depend on addition practice, slag condition, and stirring. Each plant should measure its own recovery during the trial phase. Carbon from SiC may offset recarburiser consumption (typically petroleum coke or graphite); include this offset in your cost model if applicable.
8. Common Pitfalls and How to Avoid Them
Replacing 100% of FeSi on the first trial. SiC adds carbon. If your steel grade runs close to the upper carbon limit, full substitution can cause out-of-spec heats. Start at 30% and only increase if carbon end-points remain within tolerance.
Ignoring particle size. Using 0–1 mm fines in an open ladle without enclosed feeding risks losing 20–30% of the material to off-gas. Match particle size to your addition equipment.
Skipping carbon-balance calculation. Every kilogram of 90% SiC adds roughly 0.27 kg of carbon to the bath. If your baseline FeSi practice includes a separate recarburiser addition, recalculate the total carbon budget before the trial.
Not sampling slag during the transition. The additional SiO₂ from SiC deoxidation reduces slag basicity. If the V-ratio drops too far, desulfurisation suffers. Take a slag sample after 5 and 10 trial heats.
Choosing a supplier on price alone. SiC quality varies significantly between producers. Low-purity material with high free carbon or SiO₂ content will give inconsistent recovery and may introduce unwanted tramp elements. Insist on lot-specific SGS or BV assay certificates.
9. Supplier Selection: What Procurement Managers Should Verify
When sourcing metallurgical-grade SiC for steelmaking, evaluate suppliers against these five criteria:
| Criterion | Why It Matters | ZhenAn International |
|---|---|---|
| ISO 9001:2015 certification | Ensures process control, batch traceability, and quality management system | Certified |
| Third-party assay per shipment | SGS, BV, or equivalent lab report confirming SiC content, free C, moisture, Al, S, N | Standard SGS-tested shipments |
| Annual production capacity | Suppliers above 50,000 MT/year are more likely to maintain lot-to-lot consistency | 150,000+ MT across two bases (30,000 m²) |
| Export track record | Reference ports, container loading experience, certificates of origin, Incoterms familiarity | 100+ countries served |
| Factory audit access | Supplier welcomes on-site visits and provides real-time production data | Open-factory policy; visitors welcome |
ZhenAn International Co., Limited - headquartered at Huafu Commercial Center, Wenfeng District, Anyang City, Henan Province, China - has supplied ferrosilicon and silicon carbide to mills in over 100 countries since 1994. Contact our engineering team to discuss your specific steel grade and consumption profile.
Frequently Asked Questions
Can silicon carbide completely replace ferrosilicon in steelmaking?
Silicon carbide can partially replace ferrosilicon in most EAF and BOF converter operations. Because SiC delivers both silicon and carbon simultaneously, full replacement is only feasible when the steel grade's carbon specification can accommodate the additional carbon input. In practice, a 30–50% partial substitution is the recommended starting point. Mills producing low-carbon or ultra-low-carbon grades should retain a portion of their ferrosilicon addition for independent silicon trim control. Full replacement has been validated in several Chinese converter steelmaking shops for plain carbon structural steels (Q235, Q345 equivalents), but each plant should conduct its own trial protocol before committing.
How much cost can a steel plant save by switching to silicon carbide?
Cost savings depend on three variables: the local spot price spread between ferrosilicon (FeSi75, GB/T 2272-2020) and metallurgical-grade SiC, freight, and the plant's silicon recovery rate. Based on late-2025 to mid-2026 Chinese domestic market conditions, SiC has generally traded at an 8–15% discount per equivalent silicon unit compared with FeSi75. A mill consuming 500 MT of FeSi per year that shifts 40% of its silicon units to 90% SiC could see an annual material cost reduction in the range of US $40,000–$80,000, subject to procurement terms. Plants should calculate savings using their actual delivered cost per kilogram of silicon - not per ton of material. Request a cost-model spreadsheet from our technical team for your specific operation.
Is silicon carbide suitable for all steel plants and furnace types?
Silicon carbide is most applicable in electric arc furnaces, basic oxygen furnaces, and ladle furnace refining stations - wherever both deoxidation and carbon addition are part of the process. It is less suitable for: (a) ultra-low-carbon steel grades where the carbon from SiC would require extended decarburisation; (b) induction furnaces melting scrap with tight tramp-element ceilings, because SiC purity must be verified per heat; and (c) stainless steel and high-alloy grades where silicon specifications are narrow and independent carbon control is critical. For the majority of plain carbon, low-alloy, and rebar-grade steel production, SiC is a viable partial substitute.
Which SiC grade is better for steelmaking: 88% or 90%?
SiC 88% (conforming to GB/T 2480-2022 for metallurgical-grade black silicon carbide) is the more economical choice per ton and is adequate for rebar, wire rod, and structural sections where minor impurity variation is acceptable. SiC 90% delivers higher silicon recovery per kilogram added, lower residual Al₂O₃ and free carbon, and more predictable dissolution behaviour - making it preferable for higher-value grades such as cold-heading steel, pipeline steel, or automotive sheet. Many plants use 88% for rebar and structural melts and reserve 90% for quality-critical heats. The decision should be based on your target steel's silicon and carbon tolerance bands and the cost per kilogram of recoverable silicon.
What particle size of silicon carbide should a steel plant use?
Particle size directly governs dissolution rate and recovery efficiency. The three common bands: 0–1 mm - ultrafine, dissolves within seconds; suitable for ladle additions with enclosed feeding and adequate dust extraction (risk: fines lost to off-gas). 1–3 mm - the general-purpose grade; balances dissolution speed (~15–30 seconds in a 1,600°C stirred bath) against dust loss. This is the most widely used size in ladle furnace operations. 10–50 mm - coarser lumps for BOF converter additions; slower dissolution prevents premature oxidation in the slag layer. Selection should be validated with a small-scale plant trial measuring silicon recovery at 2, 5, and 10 minutes post-addition.
How should a procurement manager evaluate a silicon carbide supplier?
Evaluate on five criteria: (1) ISO 9001:2015 certification - verifies process control and batch traceability; (2) third-party assay reports (SGS, BV, or equivalent) confirming SiC content, free carbon, moisture, and key impurities (Al, S, N) per shipment; (3) production scale - suppliers with annual capacity above 50,000 MT are more likely to maintain lot-to-lot consistency; (4) export track record - reference ports, container loading photos, certificates of origin; (5) on-site audit capability - whether the supplier welcomes factory visits. ZhenAn International meets all five: ISO 9001:2015 certified, SGS-tested shipments, 150,000+ MT annual capacity across two production bases, exports to 100+ countries, and an open-factory policy.

Start Your SiC Substitution Trial with Technical Support
Tell us your furnace type, current FeSi consumption, target steel grades, and annual tonnage. We will send a plant-specific cost model, recommended SiC grade and particle size, and a trial protocol - within one business day.
Email: market@zanewmetal.com · WhatsApp: +86 155 1882 4805
References
GB/T 2480-2022 - Conventional Abrasive - Silicon Carbide. Standardization Administration of China. https://www.codeofchina.com/standard/GBT2480-2022.html (accessed 2026-08-06)
GB/T 2272-2020 - Ferrosilicon. Standardization Administration of China. https://www.chinesestandard.net/PDF.aspx/GBT2272-2020 (accessed 2026-08-06)
Fiven ASA - "Silicon Carbide Usage in the Steel Industry." https://www.fiven.com/markets-applications/metallurgy/steel-industry/ (accessed 2026-08-06)
Miller and Company LLC - "Briquettes and Silicon Carbide for the Steel Industry." https://www.millerandco.com/briquettes-and-silicon-carbide-for-the-steel-industry/ (accessed 2026-08-06)
NIST Standard Reference Database - Silicon Carbide molecular data (molar mass 40.096 g/mol, Si 28.0855, C 12.011). https://en.wikipedia.org/wiki/Silicon_carbide (accessed 2026-08-06)
Li, H. - "The Application of SiC in Converter Steelmaking." Atlantis Press. https://download.atlantis-press.com/article/25854169.pdf (accessed 2026-08-06)
Original article: "How to Replace Ferrosilicon with Silicon Carbide | Cost-Saving Guide for Steel Plants." ZhenAn International. https://www.metal-alloy.com/info/how-to-replace-ferrosilicon-with-silicon-carbi-103455477.html (published 2026-04-07, accessed 2026-08-06)
All figures, standards, and reaction equations were verified against the cited sources as of the update date. Price ranges are indicative and based on late-2025 to mid-2026 market conditions in China as reported by SunSirs and Intratec; actual pricing is subject to contract negotiation. If you identify an error, contact our engineering team so we can correct it.